KELUM® Aluminium Hydroxide — Formulation Guidance

Hanzhong Delike New Materials Co., Ltd.
FORMULATION GUIDANCE
Document No: AL-FG-2026-01
Revision: 1.0 | Effective: July 2026
For R&D and Compounding Engineers

1. Introduction

KELUM® Aluminium Hydroxide [Al(OH)‚] is a halogen-free, non-toxic inorganic flame retardant and functional filler suitable for a wide range of polymer and coating formulations. This guidance provides practical recommendations for incorporating KELUM® into your compounding process to achieve optimal dispersion, mechanical properties, and flame retardancy.

KELUM® decomposes endothermically at 250–350 °C, releasing water vapor (34.5% LOI) that cools the substrate and dilutes combustible gases. The resulting alumina (Al‚O‚) forms a protective char layer, suppressing smoke and toxic emissions. Its fine particle size (d50: 1.2–1.8 μm for ultrafine grades) and high purity (≥ 99.6%) ensure excellent dispersibility and minimal impact on compound aesthetics.


2. Recommended Loading Levels

The table below provides recommended loading ranges (in phr — parts per hundred resin, by weight) for common polymer systems. Actual loading depends on the specific formulation, processing equipment, and performance requirements. For coating systems, loading is expressed as % PVC (Pigment Volume Concentration).

Polymer / Binder System Recommended Loading (phr) Suggested KELUM® Grade Key Benefit
PVC (Flexible & Rigid) 30 – 150 AH-B, AH-SM Smoke suppression, LOI improvement
PE / EVA (Cable Compounds) 50 – 200 AH-SM, AH-C Low smoke, halogen-free FR cable
Rubber (NR, SBR, EPDM, CR) 20 – 100 AH-B, AH-SM Flame resistance, improved tear
Epoxy (Electrical Encapsulants) 30 – 80 AH-C, AH-A Low conductivity, arc resistance
Unsaturated Polyester (SMC/BMC) 50 – 150 AH-B, AH-SM FR + low shrinkage synergy
Coatings (Waterborne & Solvent) 10 – 40% PVC AH-A, AH-B Whiteness, intumescent effect

Notes: phr = parts per hundred resin by weight. % PVC = Pigment Volume Concentration. Loading levels are starting-point recommendations; optimize via designed experiments (DOE) for your specific compound. Surface-modified grade (AH-SM) enables up to 30% higher loading vs. untreated grades in polyolefins with equivalent processability.


3. Dispersion Tips

Achieving uniform dispersion of Al(OH)‚ is critical for consistent flame retardancy and mechanical properties. Follow these best practices:

ⓘ Pro Tip: When substituting ATH for a portion of the polymer at high loadings (> 100 phr), pre-heat the filler to 80–100 °C before feeding to reduce the thermal shock on the melt and shorten cycle time. A vented extruder or vacuum devolatilization is strongly recommended to remove moisture and volatiles.

4. Processing Parameters

The table below summarizes recommended processing windows for the most common compounding methods. Adjust parameters based on your specific polymer grade, filler loading, and equipment configuration.

Parameter Twin-Screw Extruder Internal Mixer (Banbury) Two-Roll Mill
Melt Temperature 140 – 220 °C * 130 – 200 °C * 120 – 180 °C *
Residence / Mixing Time 30 – 90 seconds 4 – 10 minutes 5 – 15 minutes
Screw / Rotor Speed 200 – 600 rpm 30 – 80 rpm Friction ratio 1:1.1–1:1.3
Filler Feed Zone Downstream (side feeder) After polymer flux After band formation
Venting / Vacuum Recommended (−0.06 MPa) Ram up / vent cycle Not applicable
Target Dispersion < 50 μm agglomerates < 30 μm agglomerates < 50 μm agglomerates

* Melt temperature depends on the base polymer. For PE/EVA, target 140–180 °C; for engineering plastics (PA, PBT), target 220–260 °C. Ensure processing temperature remains below 250 °C to avoid premature decomposition of Al(OH)‚.

Twin-Screw Extruder Guidance

  • Use co-rotating, intermeshing screws
  • Configure kneading blocks in the mixing zone for dispersive mixing
  • Feed polymer in the main hopper; add filler via side feeder at barrel zone 4–5
  • Use atmospheric + vacuum venting (zones 7–8) to remove moisture
  • L/D ratio ≥ 40:1 recommended for high-fill compounds
  • Die pressure should remain stable; rising pressure may indicate screen pack fouling

Internal Mixer Guidance

  • Pre-heat chamber to 10–20 °C above polymer Tm
  • Load polymer first; after flux (torque peak), add filler in 2–3 increments
  • Monitor ram position and torque curve to judge incorporation
  • Typical fill factor: 70–80% of chamber volume
  • Drop compound at consistent batch temperature for reproducibility
  • Discharge onto a two-roll mill for sheeting and cooling

5. Compatibility

KELUM® Aluminium Hydroxide is chemically inert and broadly compatible with common formulation ingredients. The following table summarizes compatibility with typical compounding additives.

Plasticizers Fully compatible with phthalates (DOP, DINP), trimellitates (TOTM), phosphates, epoxidized soybean oil (ESBO), and polymeric plasticizers. No adverse interaction observed. Plasticizer absorption is moderate; adjust plasticizer level upward by 2–5 phr at very high filler loadings.
Heat Stabilizers Compatible with Ca/Zn, Ba/Zn, organotin, and lead-based stabilizers. The mildly alkaline nature of ATH (pH 8–9 in slurry) does not interfere with stabilizer function. Ca/Zn systems show excellent long-term color retention with ATH-filled PVC.
Other Fillers Can be used alongside calcium carbonate, talc, clay, silica, and magnesium hydroxide (MDH). ATH + MDH blends provide a broader endothermic decomposition range (ATH: 250–350 °C, MDH: 340–490 °C). ATH + antimony trioxide (ATO) shows synergistic flame retardancy when combined with halogenated systems.
Colorants Excellent whiteness retention; compatible with organic pigments, inorganic pigments, and carbon black masterbatch. The high whiteness (≥ 99.0%) of KELUM® provides a clean base for tinting and reduces TiO‚ loading.
Processing Aids Compatible with acrylic processing aids, PE waxes, stearic acid, and metal stearates (Ca/Zn stearate). Stearic acid at 0.5–1.0 phr acts as an effective dispersant and internal lubricant for ATH-filled compounds.

6. Surface Treatment

Surface modification of KELUM® Aluminium Hydroxide significantly enhances its performance in polymer compounds. The AH-SM grade is pre-treated with silane, titanate, or stearic acid coupling agents to improve filler-polymer interfacial adhesion.

Benefits of Surface Treatment

  • Reduced melt viscosity — easier processing at equal loading
  • Improved mechanical properties — higher tensile strength, elongation at break, and impact resistance
  • Lower oil absorption (16–22 ml/100g vs. 20–30 ml/100g for untreated grades)
  • Higher maximum filler loading — up to 30% more ATH can be incorporated before processability degrades
  • Better moisture resistance — reduced water uptake in the final compound
  • Improved electrical properties — lower dielectric constant and dissipation factor

Recommended Coupling Agents

  • Silane Coupling Agents (0.5–1.5 wt% on filler):
    — Vinyltrimethoxysilane (VTMO) — polyolefins, EVA
    — γ-Aminopropyltriethoxysilane (AMEO) — epoxy, PU
    — γ-Methacryloxypropyltrimethoxysilane (MEMO) — unsaturated polyester, acrylics
  • Titanate Coupling Agents (0.5–1.0 wt% on filler):
    — Isopropyl tri(dioctylpyrophosphate) titanate — general purpose
    — Isopropyl triisostearoyl titanate — polyolefins, PVC
  • Stearic Acid (1.0–2.0 wt%) — economical option for PVC and rubber compounds where ultimate mechanicals are less critical
ⓘ In-Situ Treatment Option: For customers who prefer to use untreated KELUM® grades and apply surface treatment during compounding, a silane masterbatch approach is effective: pre-blend 1 part silane with 3–5 parts ATH powder, let it adsorb for 10 minutes, then feed this concentrate with the bulk ATH into the mixer. Alternatively, inject liquid silane directly into the mixing chamber after filler incorporation. Allow 2–3 minutes additional mixing time for the coupling reaction to occur.

7. Additional Recommendations

Frequently asked questions

How much ATH should I add for LSZH compounds?

Typically 50–60 wt%; above that, surface-modified AH-SM keeps viscosity workable.

Does ATH affect mechanical properties?

At high loading, tensile and elongation fall; coupling agents and AH-SM recover much of the loss.